Fab welding · Quality

Common orbital weld defects on UHP tube and what they tell you

Most rejected orbital welds on UHP tube trace back to four causes: purge (inside discoloration), joint preparation (misalignment, gaps and incomplete penetration), weld schedule settings (bead too narrow, too wide, concave or convex) and the electrode or arc (wandering bead, arc strikes). Inspect both the outside and, with a borescope, the inside, against the acceptance criteria in your owner specification.

Defect, likely cause, what to check

Common visual faults on orbital welds in 316L tube (acceptance limits come from your specification)
What you seeLikely causeWhat to check or ask
Inside discoloration (heat tint, blue to dark oxide)Oxygen or moisture in the purge; purge stopped before the weld cooledOxygen reading before the arc, purge flow and time, leaks at fittings or dams
Incomplete penetration (no continuous inside bead)Too little heat for the wall, wrong schedule, gap or poor end squarenessEnd facing and squareness, wall thickness against the schedule, current settings
Excessive penetration or inside convexityToo much heat or too slow travel; inside purge pressure too low to support the poolSchedule levels, travel speed, purge pressure and flow restriction
Inside concavityInside purge pressure too high, pushing the weld pool outwardPurge pressure balance between inlet and outlet (restrictor or exhaust)
Misalignment (mismatch between tube ends)Poor clamping, out-of-round tube, mixed tube sourcesFit-up in the head clamps, tube ovality, same tube specification on both sides
Meandering bead (bead wanders off the joint line)Electrode not centred on the joint, worn or bent tungsten, or a different sulfur content between the two tube or fitting heatsTungsten position and condition; heat numbers of both components
Arc strike, porosity or crackContamination, wet gas, bad electrode, poor cleaningCleaning, gas line condition, electrode storage

Purge limits: high-purity work needs very low oxygen in the purge before the arc starts. Equipment makers’ guidance and owner specifications set limits in the low single-digit ppm range or below for UHP work; use the number in your specification, not a general figure.

Use the faults in hiring and onboarding

  • In the interview, show photos of two or three faults and ask the candidate what caused them and how they would fix the schedule or setup.
  • In the weld test, ask for borescope images of every coupon, not only the best one.
  • In the first weeks, review the new hire’s sample welds and production welds against the weld log, and look for repeated faults of one type — they point to a habit, not bad luck.

What a good orbital welder does before every weld

  1. Faces and checks tube ends for squareness and burrs.
  2. Checks the tungsten condition and position.
  3. Purges and reads oxygen before striking the arc.
  4. Welds a sample coupon when the specification requires it and checks it inside and out.
  5. Records the weld in the log with welder ID and material information.

Frequently asked questions

Is any inside discoloration acceptable?

That depends on the owner specification. UHP gas systems usually accept very little or none; some specifications use a colour reference. Use the acceptance criteria in your specification.

Do we need to borescope every weld?

Your specification decides the inspection rate. Borescoping sample coupons is standard practice, and many fab specifications require inside inspection of a share or all of production welds.

Do repeated defects mean the welder is not qualified?

Not necessarily, but they show a pattern worth addressing. Check whether one cause, such as purge or end preparation, explains them, and retrain or retest as your QA procedure requires.

Have a fab scope that needs these trades?

Requests are in preview: you can fill in the request form, but it does not submit yet. Email WELDK with your roles, site country and start window.